闀灞傜殑鎬ц川錛氫竴鑸帤搴﹀ぇ綰?/span>2.0-3.0 渭m錛涙懇鎿︾郴鏁板皬浜?0.15銆傦紙鍏稿瀷涓猴細(xì)0.05-0.10闂達(dá)級(against WC/Co ball)錛涚‖搴?/span>Hp > 1,200kg/mm2 錛涙繁鐏伴粦鑹詫紱鍒掔棔綺樻帴鍔涳細(xì)澶т簬60N錛涚浉瀵圭(鎹熺巼錛?/span>2E-16 m3/Nm (WC-6%Co ball 脴5mm, 80 N test 脴8mm track, 477rpm, 200mms-1)銆?/span>
路 MoS2鍩洪晙灞備竴鑸帤搴﹀ぇ浜?/span>1.0 渭m錛涙懇鎿︾郴鏁扮害涓?/span>0.05 鍒?0.10涔嬮棿(against WC/Co ball)錛涘湪150kgf鐨勬礇姘忕‖搴﹁鍘嬪ご鍘嬪叆錛岄晙灞備笉鑴辮惤錛?/span>>HF2錛夛紝紜害綰?950-1050 VHN錛涙繁鐏拌壊錛涘垝鐥曠矘鎺ュ姏錛氬ぇ浜?/span>60N錛涚浉瀵圭(鎹熺巼錛?/span>2E-16 m3/Nm (WC-6%Co ball 脴5mm, 40 N test 脴8mm track, 477rpm, 200mms-1)銆?/span>
路 鈥oST : Properties of coating
CrN 闀灞?/span>
CrN: 闀灞傜‖搴f>2000HV錛岄晙灞傚帤搴?gt;3寰背錛涚粨鍚堝姏錛氬湪150kgf鐨勬礇姘忕‖搴﹁鍘嬪ご鍘嬪叆錛岄晙灞備笉鑴辮惤錛?gt;HF2錛夛紱 鏍囧噯鍒掔棔璇曢獙錛歀c>60N錛涢晙灞傚墠鍚庣殑琛ㄩ潰綺楃硻搴﹀鍔犲糝a鈮?.01寰背錛岄暅闈㈡晥鏋溿?/span>
CrN coating, the hardness of the coating: Hf>2000Hv, the thickness of the coatings: >3.0um. The adhesion of the coatings: >HF2. And Lc > 60N with Scratch system. The Roughness of the coating Ra<0.01